Differential Scanning Calorimetry

概要

Source: Danielle N. Beatty and Taylor D. Sparks, Department of Materials Science and Engineering, The University of Utah, Salt Lake City, UT

Differential scanning calorimetry (DSC) is an important measurement to characterize thermal properties of materials. DSC is used primarily to calculate the amount of heat stored in a material as it heats up (heat capacity) as well as the heat absorbed or released during chemical reactions or phase changes. However, measurement of this heat can also lead to the calculation of other important properties such as glassy transition temperature, polymer crystallinity, and more.

Due to the long, chain-like nature of polymers it is not uncommon for polymer strands to be entangled and disordered. As a result, most polymers are only partially crystalline with the remainder of the polymer being amorphous. In this experiment we will utilize DSC to determine polymer crystallinity.

手順
  1. Turn on the machine and allow it to warm up for about an hour.
  2. Check to ensure the compressed nitrogen tank and liquid nitrogen tank are both full and the valve connecting them is open. The compressed nitrogen pressure flow is set at 10 psi by the adjustment knobs on the regulator.
  3. Prepare two empty pans. Poke a small hole in the lid of each and seal by using the crimping press. Remove the three furnace lids and place the pans on the two circular sensors within the furnace. Replace all three lids.
  4. Click o

Log in or to access full content. Learn more about your institution’s access to JoVE content here

結果

Figure 3 shows the result of a DSC percent crystallinity sample scan on a polybutylene terephthalate (PBT) polymer sample. The result is displayed as a DSC power reading (in milliwatts per milligram of sample) verses time. The power reading, the blue trace in Figure 3, indicates how much additional power was required to change the temperature of the sample pan in comparison to the empty reference pan. The temperature program is a

Log in or to access full content. Learn more about your institution’s access to JoVE content here

申請書と概要

Differential scanning calorimetry is a technique used to determine many thermal properties of materials, such as heat of melting, heat of crystallization, heat capacity, and phase changes. DSC measurements can also be used to calculate additional material properties including glassy transition temperature and polymer percent crystallinity. The DSC requires very small samples that must conform to the size and shape of the pans used in the machine and is based on a differential heat comparison between an empty reference an

Log in or to access full content. Learn more about your institution’s access to JoVE content here

タグ
Differential Scanning CalorimetryDSCThermal PropertiesMaterialsPolymersMeasurement TechniqueSample PanReference PanTemperature SensorsHeatersEnergy FlowPhase ChangeReactionPolymer Phase TransitionsPercent CrystallinityCrystalline PolymersAmorphous PolymersMeltingGlass Transition

スキップ先...

0:08

Overview

1:26

Principles of DSC Analysis of Polymers

3:51

DSC Baseline Measurement

6:52

DSC Sample Measurement

8:21

Analysis of the DSC Data

9:33

Applications

11:29

Summary

このコレクションのビデオ:

article

Now Playing

Differential Scanning Calorimetry

Materials Engineering

36.2K 閲覧数

article

光学材料グラフィー パート 1: サンプル調製

Materials Engineering

15.3K 閲覧数

article

光学材料学 パート2:画像解析

Materials Engineering

10.9K 閲覧数

article

X線光電子分光法

Materials Engineering

21.4K 閲覧数

article

X線回折

Materials Engineering

87.5K 閲覧数

article

集束イオンビーム

Materials Engineering

8.8K 閲覧数

article

方向固化と位相安定化

Materials Engineering

6.5K 閲覧数

article

熱拡散率とレーザーフラッシュ法

Materials Engineering

13.1K 閲覧数

article

薄膜の電気めっき

Materials Engineering

19.5K 閲覧数

article

拡張測定による熱膨張の解析

Materials Engineering

15.5K 閲覧数

article

電気化学インピーダンス分光法

Materials Engineering

22.9K 閲覧数

article

セラミックマトリックス複合材料とその曲げ特性

Materials Engineering

8.0K 閲覧数

article

ナノ結晶合金とナノ粒サイズ安定性

Materials Engineering

5.1K 閲覧数

article

ヒドロゲル合成

Materials Engineering

23.4K 閲覧数

JoVE Logo

個人情報保護方針

利用規約

一般データ保護規則

研究

教育

JoVEについて

Copyright © 2023 MyJoVE Corporation. All rights reserved