Using Differential Scanning Calorimetry to Measure Changes in Enthalpy

Visão Geral

Source: Laboratory of Dr. Terry Tritt — Clemson University

Differential Scanning Calorimetry (DSC) is a method of thermodynamic analysis based on heat-flux method, wherein a sample material (enclosed in a pan) and an empty reference pan are subjected to identical temperature conditions. The energy difference that is required to maintain both the pans at the same temperature, owing to the difference in the heat capacities of the sample and the reference pan, is recorded as a function of temperature. This energy released or absorbed is a measure of the enthalpy change (ΔΗ) of the sample with respect to the reference pan.

Procedimento

1. Baseline Measurement

  1. Controller, Measuring unit, Computer system, Thermostat approximately 60 min. before starting the measurement. Purge gases must be connected to the system.
  2. Place two empty crucibles (with lid) into the sample carrier. The crucible material may be chosen based on the temperature range to be measured.
  3. Move the furnace to measuring position.
  4. Adjust the measuring conditions (gas, vacuum).
  5. Start the measurement program.
  6. Proceed to create a b

Log in or to access full content. Learn more about your institution’s access to JoVE content here

Resultados

ZnO formation via Decomposition of ZnCO3

The change in enthalpy per degree, at constant pressure is equivalent to the heat capacity of a material at constant pressure given by Equation 1. The enthalpy change is obtained by estimating the area under the curve between two temperature limits given by Equation 2.

(Equation 1)

Log in or to access full content. Learn more about your institution’s access to JoVE content here

Aplicação e Resumo

A major application area of DSC is the glass transition (Tg) in amorphous polymers, in which the material changes from a rigid glassy state to a viscous liquid state. Pharmaceutical research on nano-particles is also an emerging field, where the DSC has been used to quantify amorphous or crystalline phase in nano-solids. A review of DSC techniques on applications in biology and nano-science has been provided by Gill et al.3 Nanostructured lipid carriers (NLC) have potential applications in

Log in or to access full content. Learn more about your institution’s access to JoVE content here

Referências
  1. Robinson, J.W., Skelly Frame, E.M., Frame, GM. Undergraduate Instrumental Analysis. Marcel Decker, New York, NY. (2005).
  2. Liu, S., Li, C., Yu, J., Xiang, Q., Improved visible-light photocatalytic activity or porous carbon self-doped ZnO nanosheet-assembled flowers. CrystEngComm. 13, p 2533 (2011).
  3. Gill, P., Tohidu Moghadam, T., Ranjbar, B.  Differential Scanning Calorimetry Techniques: Applications in Biology and Nanoscience. Biomolecular Techniques. 21, 167-193 (2010).
Tags
Differential Scanning CalorimetryEnthalpyEnergy ChangesChemical ReactionsThermodynamicsConstant PressureExothermic ReactionsEndothermic ReactionsSafetyEfficiencyExperimentHeat FlowOxide DecompositionCarbonate Decomposition

Pular para...

0:00

Overview

1:23

Principles of Enthalpy

3:48

DSC Baseline Measurement

5:04

DSC Reference Measurement

6:22

Sample Measurement

7:10

Analysis of the DSC Data

8:42

Applications

10:56

Summary

Vídeos desta coleção:

article

Now Playing

Using Differential Scanning Calorimetry to Measure Changes in Enthalpy

General Chemistry

44.3K Visualizações

article

Vidraria de laboratório comuns e seus usos

General Chemistry

651.0K Visualizações

article

Soluções e Concentrações

General Chemistry

271.7K Visualizações

article

Determinando a densidade de um sólido e um líquido

General Chemistry

552.9K Visualizações

article

Determinação de composição percentual em massa em uma solução aquosa

General Chemistry

382.7K Visualizações

article

Determinação da Fórmula Empírica

General Chemistry

178.1K Visualizações

article

Determinação das Regras de Solubilidade de Compostos Iônicos

General Chemistry

140.8K Visualizações

article

Usando um medidor de pH

General Chemistry

343.3K Visualizações

article

Introdução à Titulação

General Chemistry

421.8K Visualizações

article

Lei dos gases ideais

General Chemistry

77.5K Visualizações

article

Determinação espectrofotométrica de uma constante de equilíbrio

General Chemistry

157.9K Visualizações

article

Princípio de Le Châtelier

General Chemistry

262.8K Visualizações

article

Depressão do ponto de congelamento para determinar um composto desconhecido

General Chemistry

159.4K Visualizações

article

Determinação das Leis de Velocidade e da Ordem de Reação

General Chemistry

195.4K Visualizações

article

Complexos de Química de Coordenação

General Chemistry

90.6K Visualizações

JoVE Logo

Privacidade

Termos de uso

Políticas

Pesquisa

Educação

SOBRE A JoVE

Copyright © 2025 MyJoVE Corporation. Todos os direitos reservados